I. Visual Inspection: Immediately assess the basic weld quality. After welding, once the weld has cooled to a safe touch (usually over 20 minutes), a 100% visual inspection should be performed immediately. This is the most basic and crucial initial assessment.
The rolled edge should be full, uniform, and a continuous semi-circular shape, with a height between 1 and 2 mm. If the rolled edge is too low, it may indicate insufficient heating; if too high, it suggests excessive pressure; asymmetry reflects poor alignment or a tilted heating plate.
Joint alignment must be good. The axes of the two pipes should be aligned, and the misalignment should not exceed 10% of the pipe wall thickness (e.g., ≤0.6 mm for a 6 mm wall thickness).
Rolled edge trimming and back bend inspection (sampling): Cut the rolled edge every 50 mm to make a 180° back bend. There should be no cracks, fissures, or lack of fusion at the center line. Delamination or exposed fusion lines indicate poor internal fusion.
✅ It is recommended to retain original photos and welding parameter records for each weld joint to ensure quality traceability.
II. Non-destructive Testing: A Key Method for Detecting Hidden Defects
For critical projects or buried pipelines, visual inspection alone is insufficient to ensure safety; non-destructive testing (NDT) techniques are necessary to identify internal defects.
Phase-array ultrasonic testing (PAUT) combined with TOFD: This is currently the most effective NDT method for HDPE welds. It can clearly identify defects such as incomplete fusion, inclusions, and cold welds. It offers deep detection and high resolution, making it suitable for thick-walled pipelines.
Pressure testing: For double-welded structures (such as geomembranes), pressure can be applied to 250 kPa and held for 3-5 minutes. If the pressure does not drop, it is considered (qualified).
Electrical spark testing: Suitable for extrusion welds in seepage prevention projects. After pre-embedding copper wire, a high-voltage probe is used for scanning; the appearance of sparks indicates the presence of a leak.
⚠️ Note: High-frequency ultrasound is not suitable for HDPE materials because its acoustic impedance is similar to that of a wedge. Low-frequency ultrasound or PAUT technology is recommended. III. Pressure Testing: The Ultimate Means of Verifying the Overall System Sealing
A hydrostatic test must be conducted after the weld has completely cooled and been allowed to stand for 24 hours to ensure sufficient crystallization in the weld zone and achieve optimal mechanical properties.
The test pressure should not be less than 1.5 times the pipeline's working pressure, and must not be lower than 0.80 MPa.
Clean water must be used as the medium; air pressure testing is strictly prohibited as a substitute for hydrostatic testing.
The pressure testing process is divided into a pre-test and a main test phase: In the pre-test, the pressure is raised to the test pressure and held for 30 minutes to check for leaks; In the main test phase, the pressure is reduced by 10%~15%, and the leakage is observed to ensure it is within the allowable range.
✅ Passing Standard for Pressure Testing: No leakage or significant pressure drop during the pressure holding period; the corrected pressure drop should not exceed 133 Pa/h.
IV. Destructive Testing: Used for Process Verification or Dispute Arbitration
Before construction or when quality is in doubt, a small number of weld joints can be sampled for destructive testing to directly verify the weld strength.
Tensile peel test: Tests the tensile strength of the weld. If fracture occurs in the base material rather than the weld, the weld quality is reliable.
Short-term hydrostatic strength test: The sample is pressurized to a specified value and held under pressure to examine its pressure resistance.
🔍 Comprehensive recommendation: Daily construction should focus on visual inspection + non-destructive testing + hydrostatic testing after 24 hours as the core process to ensure the safety and reliability of every weld.